ISO 9001 Certified·Domestic Manufacturer — Houston, TX
Hot-shot line open832-446-3442
Innovation FastenersInnovation Fasteners
HomeEmergency / Hot-shot 24/7ContactGet a Quote
Nickel alloys · ASTM B637

Waspaloy® (UNS N07001)

The gas-turbine superalloy for bolting that runs hotter than Inconel 718 can take: nickel-chromium-cobalt, age hardened by titanium and aluminium, 160 ksi tensile and stress-rupture rated at 1500 °F.

UNS N07001Alloy Waspaloy · W.Nr. 2.4654Type Precipitation-hardening nickel-chromium-cobalt superalloy with Mo, Ti and Al
Material overview

What Waspaloy is.

Waspaloy is a wrought nickel-base superalloy with 18 to 21 percent chromium, 12 to 15 percent cobalt and 3.5 to 5 percent molybdenum, strengthened by gamma-prime precipitates of titanium and aluminium. It was developed for aircraft gas-turbine engines and is used for turbine discs, shafts, rings, casings and the fasteners that hold them together. It keeps its strength hotter than Inconel 718: ASTM B637 proves Waspaloy by a stress-rupture test at 1500 °F, against 1200 °F for 718.

We machine Waspaloy studs, bolts, nuts and components from certified ASTM B637 or AMS bar, supplied with the solution, stabilizing and precipitation-hardening treatment of the specification and PMI on every lot.

Get a QuoteDownload the Waspaloy data sheet (PDF)
Tensile, fully heat treated160 ksi min
Yield, fully heat treated110 ksi min
Hardness310 HBW min
Stress rupture33 ksi at 1500 °F, 100 h min
Chromium18.00–21.00 %
Cobalt12.00–15.00 %
Nominal composition
Ni balance ≈ 56.1%Cr ≈ 19.50%Co ≈ 13.50%Mo ≈ 4.25%Ti ≈ 3.00%Al ≈ 1.40%Fe ≈ 1.00%Mn ≈ 0.50%C, Si, P, S, Zr, B, Cu trace

Midpoints of the specification ranges, for orientation only. Limits are in the table below.

Specifications & technical data

Chemical composition.

Download the data sheet (PDF) →
Chemical composition — Waspaloy (UNS N07001)
ElementSymbolMin %Max %
CarbonC0.030.10
ManganeseMn—1.00
SiliconSi—0.75
PhosphorusP—0.030
SulfurS—0.030
ChromiumCr18.0021.00
CobaltCo12.0015.00
MolybdenumMo3.505.00
TitaniumTi2.753.25
AluminiumAl1.201.60
ZirconiumZr0.020.12
BoronB0.0030.01
IronFe—2.00
CopperCu—0.50
NickelNibalance—

Values per ASTM B637-16 Table 1 (verified against the specification). Confirm the edition called out on your purchase order with our estimating team.

Physical properties (typical)
Density0.296 lb/in³ (8.20 g/cm³)
Modulus of elasticity30.9 × 10⁶ psi (213 GPa)
Thermal expansion (70–800 °F)7.6 µin/in·°F
Melting range2425–2475 °F (1330–1360 °C)
Specifications & technical data

Mechanical properties.

Mechanical properties — Waspaloy (UNS N07001)
ConditionTensile strength, min (ksi)Yield strength 0.2% offset, min (ksi)Elongation, min (%)Reduction of area, min (%)Hardness
Solution treated + stabilized + precipitation hardened1601101518310 HBW min

Values per ASTM B637-16 Table 3 (verified against the specification), which marks the elongation and reduction-of-area figures with its note B, “Forgings”. Confirm the edition called out on your purchase order with our estimating team.

Stress-rupture requirement — Waspaloy per ASTM B637 Table 4
Test temperatureStress (ksi)Time to rupture, min (h)Elongation, min (%)
1500 °F (816 °C)331005

Values per ASTM B637-16 Table 4 (verified against the specification). Confirm the edition called out on your purchase order with our estimating team.

Heat treatment — Waspaloy per ASTM B637 Table 2
StepCycle
Solution treatment (recommended)1825–1900 °F (996–1038 °C), hold 4 h, oil or water quench
Stabilizing treatment (recommended)1550 ± 25 °F (843 ± 14 °C), hold 4 h, air cool
Precipitation hardening1400 ± 25 °F (760 ± 14 °C), hold 16 h, air cool or furnace cool

Values per ASTM B637-16 Table 2 (verified against the specification). Confirm the edition called out on your purchase order with our estimating team.

Heat treatmentSolution treat at 1825–1900 °F for 4 hours and oil or water quench, stabilize at 1550 ± 25 °F for 4 hours and air cool, then age at 1400 ± 25 °F for 16 hours and air or furnace cool (B637 Table 2). B637 lists the condition as solution treated, stabilized and precipitation hardened.
Standards

Specifications that apply.

ASTM B637Precipitation-hardening nickel alloy bars, forgings and forging stock (UNS N07001, formerly Grade 685)
SAE AMS 5704 / 5706 / 5707 / 5708 / 5709Aerospace specifications for Waspaloy rod, bar and forgings
W.Nr. 2.4654European material number
Forms we supply

How Waspaloy ships from Houston.

  • Studs and stud bolts
  • Hex, heavy hex and 12-point bolts
  • Nuts and washers
  • Machined components from certified bar
Companion grades
Stronger below 1200 °FInconel 718 (UNS N07718)
Turbine bolting relativeNimonic® 80A (UNS N07080)
Iron-base turbine boltingASTM A453 Grade 660 (A-286)
45 products in this grade

Waspaloy fasteners we make.

All products →

Every item is manufactured to your drawing or standard in Waspaloy, imperial or metric, with an EN 10204 3.1 certificate.

Where Waspaloy is used
Gas turbine case, flange and rotor boltingTurbine discs, shafts, rings and sealsAircraft engine and aerospace hot-section hardwareIndustrial gas turbine and power-generation fastenersHigh-temperature fasteners beyond the range of Inconel 718
The buyer’s guide

What is Waspaloy?

Waspaloy is an age-hardenable nickel-base superalloy made for the hot end of gas turbines. Chromium gives it oxidation resistance, cobalt and molybdenum strengthen the matrix, and titanium and aluminium form the gamma-prime precipitates that keep it strong when it is hot. Published alloy data describe very good strength to about 1800 °F and good resistance to gas-turbine combustion gases to about 1600 °F. In ASTM B637 it is UNS N07001, formerly Grade 685; aerospace drawings usually call it out by an AMS number.

For fasteners, Waspaloy is the step up when a joint runs too hot for Inconel 718. It is weaker than 718 at room temperature, 160 ksi tensile against 185 ksi, but B637 tests it in stress rupture at 1500 °F where 718 is tested at 1200 °F.

Waspaloy, Inconel 718 or Nimonic 80A?

  • Inconel 718: 185 ksi tensile and 150 ksi yield, stress-rupture tested at 100 ksi and 1200 °F. The stronger and usually the more economical choice while the joint stays at or below about 1200 °F.
  • Waspaloy: 160 ksi tensile and 110 ksi yield, stress-rupture tested at 33 ksi and 1500 °F for 100 hours. The choice for hotter joints.
  • Nimonic 80A: 135 ksi tensile and 90 ksi yield, stress-rupture tested at 47 ksi and 1400 °F. A simpler nickel-chromium alloy without the cobalt and molybdenum, common on European and turbine OEM drawings.

Ordering Waspaloy fasteners

  • State the alloy (Waspaloy, UNS N07001), the specification (ASTM B637 or the AMS number on the drawing) and the heat-treated condition.
  • B637 asks the purchaser to name any partial stage of heat treatment wanted on the material, so say whether parts are to arrive fully heat treated.
  • Send the drawing or the thread, length and quantity. Waspaloy is made to order, so ask for the lead time with the quote.

Testing, certification and marking

  • Tensile and hardness tested to ASTM B637 Table 3; Table 4 also requires a stress-rupture test (1500 °F, 33 ksi, 100 h minimum)
  • EN 10204 3.1 material test report with heat number and chemistry; 3.2 witness available
  • PMI verification standard on nickel alloys

Need Waspaloy to a drawing? Need it tonight?

24/7 hot-shot manufacturing · 832-446-3442
Get a Quote